⚛️Atomic Layer Deposition
HackerFab DIY Low-Cost Atomic Layer Deposition (ALD) Tool
Important links:
Build Guide (coming by end of 2026)
Preface
These pages will present the current proposed machine design plan and the work completed to date for our vertically-aligned, cold-walled reaction chamber ALD machine for the Hacker Fab at CMU.
You may read the status updates from the 2025-26 academic year, along with the Summer 2025 + Spring 2025 + Fall 2024 updates, by navigating to the appropriate subpages in the sidebar. Please note that there were significant changes to the design of the chamber, precursor storage, and control systems from the 2024-25 to 2025-26 academic years; those aiming to replicate these efforts are recommended to read the most recent updates to better understand the current state of the system.
What follows is an overview of our ALD system including a literature review and miscellaneous background research. Once the tool is fully online and operational by the end of 2026, we intend to publish a formal build guide to GitBook.
Introduction
We are building a low cost Atomic Layer Deposition machine for the Hacker Fab to achieve improved gate dielectrics, which will help us achieve our goal of a CMOS process as well as improve our capability in performing thin-film research. Our design work on it will be open-source, and we hope other labs can use our work to make their own ALDs at a fraction of the cost of commercial alternatives. We are building our ALD to fit 4" wafers so that it can be brought into the nanofab, which will help us lower the barrier to entry for researching thin film deposition and new materials. Although 4" is much larger than anything we are currently using in the Hacker Fab at CMU, this larger size will make it useful to a larger audience.
Our work thus far has been focused on machine design, largely drawing from two papers on “DIY” ALD machines: “Design Of Atomic Layer Deposition Reactors For The Deposition Of Nanoparticle Embedded Thin Films” by Michael Lubitz, and “Homebuilt Reactor Design and Atomic Layer Deposition of Metal Oxide Thin Films” by Pamburayi Mpofu. Each of these papers describes their machine design followed by some process development where they describe the settings (i.e. temperatures and precursors deposition times) used in their initial depositions.
Precursor Selection
Oxide of interest
For the current system we aim to deposit Indium-Tin Oxide. Indium Tin Oxide (ITO) is a versatile material widely recognized for its excellent electrical conductivity and optical transparency. These properties make ITO a promising candidate for advanced applications, particularly as a channel material in thin-film transistors (TFTs). Its high carrier mobility and tunable electrical characteristics offer significant potential for improving TFT performance in display technologies and flexible electronics. Additionally, ITO thin films are of great interest in materials and thin-film research due to their unique combination of metallic and semiconducting properties. This makes them an ideal system for exploring novel deposition techniques, optimizing film uniformity, and investigating structure-property relationships.
The precursors for the metals were chosen based on their feasibility to react with water vapor as the oxidizer. The precursors chosen are Trimethyl Indium (TMIn) for Indium and Tetrakis(dimethylamino) Tin (TDMASn) for Tin with Nitrogen carrier gas. They have been shown to be used for ALD and CVD processes with water as the oxidizer in literature. As a starting point our aim would be to reproduce the results achieved in [Zhang et al.]. The process parameters highlighted in the paper are as follows (substrate temperature: -225C):
Oxide
Bubbler temperature
Pulse time
Co-reactant pulse time
Process pressure
Purge time
In2O3
60oC
0.625s
0.75s
100 mTorr
10s
SnO2
60oC
2s
1s
100 mTorr
30s
For the first attempts at deposition however, the research group at CMU will attempt to deposition Hafnium Oxide (HfO2), as this process is well-documented in the CMU Nanofab. Then, the group will attempt to deposit more complex oxides such as ITO.
Safety Considerations
Most precursors and specifically metal organic precursors used for CVD and ALD processes tend to be pyrophoric (i.e. thermally unstable and spontaneously ignite on exposure to air)m thus necessitating safety measures.
Material Considerations
Compatibility with the precursors and byproducts produced during reaction are important to consider when selecting components for the delivery system. For our given precursors the chemical groups for which we checked compatibility are: 1) ability to handle pyrophoric materials, 2) ability to resist corrosion due to water vapor, 3) compatibility with methane (by product of TMIn reaction with water) and dimethylamine gas (by product of TDMASn reaction with water)
The compatibility of o-ring materials was checked on the following sources: (1) (2)
Specific choices:
Stainless Steel Tubing
Aflas O-rings - conventionally used Viton O-rings are incompatible with dimethylamine
Aluminum vacuum chamber
Stainless steel bellow hose
Vacuum pump - Although the vacuum pump manufacturer warns against using the pump with pyrophoric gases, this caution can be safely disregarded in our case. Since we will be working with extremely dilute concentrations of these gases, the risk of combustion or hazardous reactions is significantly minimized. The low concentration ensures that the gases remain well within safe limits, allowing for the pump's use without compromising safety or performance.
Sourcing Precursors
Given the safety considerations involved in handling the pyrophoric precursors, the sourcing of materials for ITO deposition is managed by the Claire & John Bertucci Nanotechnology Laboratory staff. They ensure that all necessary precautions are taken during the procurement, handling, and storage of the chemicals. The required precursors have been ordered from Strem Chemicals, a trusted supplier known for providing high-quality materials for advanced research and industrial applications. TMIn, TDMASn
Key Components
ALD precursors and co-reactants are self-limiting
Precursor and co-reactant selection
Have to be reactive with the surface groups
Volatility, thermal stability, and reactivity have to be high
Different ways to deliver the precursor to the chamber
Chemical composition
Checking if the intended materials are being deposited through X-ray photoelectron spectroscopy (XPS) or four-point probe conductivity measurement
Optimization of the parameters
Chemical composition and stoichiometry will determine the final material properties
Thickness control
Want to deposit the same amount of material in each cycle
Thickness is determined per cycle (growth per cycle or GPC)
Keep track of material increase during deposition and deposit multiple samples with a varying number of cycles (Thickness vs. ALD cycles)
Focus of thicker films over 15 nm
Determining film thickness:
Spectroscopic ellipsometry
Number of deposited atoms (rutherford backscattering spectroscopy)
Deposited mass (quartz-crystal microbalance or QCM)
Saturation
Need to optimize precursor dosing time, precursor purging time, co-reactant dosing time, and co-reactant purging time (two-step process)
Choose a relatively long time for three of the four while varying the fourth
Confirm saturation when increasing the dosing or purging time does not increase or decrease the GPC any more (do with all steps of the procedure)
Phenomena that deviate the saturation curve
Precursor condensation and decomposition (precursor curve)
Too short co-reactant dosing times (impurity incorporation)
Too short purging times (parasitic components impacting conformality and uniformity
Too long dosing and purging times can slow down the process

Material properties
Optical properties (refractive index, absorption coefficient)
Electrical properties (resistivity, carrier density, mobility)
Surface morphology (roughness, crystallinity)
Temperature dependence
ALD window where the GPC is nearly constant for reliability and repeatability despite slight change in temperature
Constant GPC is not necessary but verifying saturation is important for all varied temperatures
Temperature dependent GPC exist but show saturating ALD behavior over a wide temp. range

Uniformity
Verified saturation in one area doesn’t mean dosing is sufficient everywhere
Place the largest fitting substrate into the chamber and check for thickness variation as well as material properties
Thickness uniformity may be good but the resistivity might vary significantly over the substrate
Conformality
Ability to deposit on 3D structures with no variation in thickness (trenches or vias)
Check for conformality
Deposit a vertical trench or via with a certain aspect ration (AR = height/width)
After deposition, calculate the ratio at different locations in comparison to the thickness at the surface
There is also the Pillar Hall aspect ratio test

Nucleation behavior
Different film growth behavior from beginning to end
Linear growth, accelerated growth, and delayed growth
Nucleation behavior can affect material properties (defects, pinhole density, crystalline structure, and film resistivity)
Nucleation behavior depends on the growth mode
Island growth forms isolated clusters that will eventually grow into a continuous film
Layer-by-layer growth
Growth mode depends on the difference in surface energy (substrate and deposited film)
GPC increase after crystallization after a certain thickness
Other important aspects
Stability of the films over time and sensitivity to the environment
Reproducible film thickness and properties
Avoid overdosing and required precursor dosing depends on the surface area of the substrate (larger when working with 3D substrates)
Precursors can degrade after prolonged heating so turn off the heating when not depositing
References
Z. Zhang et al., "Atomically Thin Indium-Tin-Oxide Transistors Enabled by Atomic Layer Deposition," in IEEE Transactions on Electron Devices, vol. 69, no. 1, pp. 231-236, Jan. 2022, doi: 10.1109/TED.2021.3129707.
“Design Of Atomic Layer Deposition Reactors For The Deposition Of Nanoparticle Embedded Thin Films” by Michael Lubitz
"Homebuilt Reactor Design and Atomic Layer Deposition of Metal Oxide Thin Films" by Pamburayi Mpofu
Last updated