> For the complete documentation index, see [llms.txt](https://docs.hackerfab.org/home/llms.txt). Markdown versions of documentation pages are available by appending `.md` to page URLs; this page is available as [Markdown](https://docs.hackerfab.org/home/standard-operating-procedures/patterning-sop-stepper-v2/spin-coating-sop-rev-2-uwaterloo.md).

# Spin Coating SOP Rev 2 (UWaterloo)

## Purpose

To apply a uniform photoresist coating on silicon wafers using a calibrated spin-coater for microfabrication and lithography processes.

This SOP supports HackerFab lithography workflows targeting <10 µm features, consistent with recent calibration results.

Currently, our spin coater has an error tolerance of <0.1%.

<figure><img src="/files/j14PoKQtZBLbv6ofNKt8" alt="" width="375"><figcaption></figcaption></figure>

## Scope

Applies to:

* Silicon wafers (1cm x 1cm diced samples)
* Positive photoresist
* HackerFab custom spin-coater

Used before:

* UV lithography
* Pattern transfer
* Etching or lift-off

## Equipment & Materials

### Equipment

* HackerFab calibrated spin-coater
* Hot plate
* Micropipette or resist dropper
* Wafer tweezers
* Timer
* Fume hood or wet lab bench

### Materials

* Silicon wafers
* Photoresist (AZ-P4620)
* Acetone
* IPA
* DI water
* He gas

## Safety Precautions

Work inside fume hood. Wear gloves, goggles, lab coat.

Photoresist solvents are flammable and toxic.

If using developers or etchants later (KOH, HF etc.), follow separate SOPs.

Dispose waste in labeled resist-waste container.

## Process Parameters

(Fill based on your calibrated spin-coater data)

| Step        | Parameter      | Typical Value |
| ----------- | -------------- | ------------- |
| Clean       | DI water rinse | 10s           |
| Clean       | Acetone rinse  | 10s           |
| Clean       | IPA rinse      | 10s           |
| Dry         | He blow dry    | Until dry     |
| Spin step 1 | Spread speed   | 500 rpm, 5s   |
| Spin step 2 | Final speed    | 5000 rpm, 30s |
| Soft bake   | Temp; Time     | 100°C; 1min   |

## Procedure

See <https://www.youtube.com/watch?v=g-riji6kyWk> for video tutorial on Spin Coater usage.

### Wafer Cleaning

1. Rinse wafer with DI Water.
2. Rinse wafer with acetone.
3. Rinse with IPA.
4. Blow dry with Helium.
5. Inspect wafer for particles.

### Spin Coating

1. Place wafer on spin-coater chuck.
2. Dispense \~1 mL photoresist at wafer center.
3. Run spin program:
   * Spread: 500 rpm for 5 s
   * Spin: 4500-5000 rpm for 30 s
4. Stop spin-coater.
5. Remove wafer carefully.

### Soft Bake

1. Place wafer on hot plate at 100 °C.
2. Bake for 60 s.
3. Cool wafer on clean surface.

## &#x20;Expected Results

* Uniform resist thickness.
* No streaks or bubbles.
* Good adhesion.
* Compatible with UV lithography, achieving <10 µm features.

## Troubleshooting

| Problem                 | Cause                                  | Fix                                           |
| ----------------------- | -------------------------------------- | --------------------------------------------- |
| Spin Coater Not Booting | Boot failure                           | Unplug and replug cable                       |
| Insufficient Power      | USB source cannot provide enough power | Use a USB-C PD source rated for more than 15W |
| Edge bead               | Too much resist                        | Use less resist volume                        |
| Streaks                 | Dirty wafer                            | Improve cleaning                              |
| Non-uniform thickness   | RPM mismatch                           | Recalibrate spin-coater                       |
| Bubbles                 | Moisture                               | Dehydrate bake wafer                          |

## &#x20;Notes

* Use tachometer-verified RPM values


---

# Agent Instructions
This documentation is published with GitBook. GitBook is the documentation platform designed so that both humans and AI agents can read, navigate, and reason over technical content effectively. Learn more at gitbook.com.

## Querying This Documentation
If you need additional information that is not directly available in this page, you can query the documentation dynamically by asking a question.

Perform an HTTP GET request on the current page URL with the `ask` query parameter, and the optional `goal` query parameter:

```
GET https://docs.hackerfab.org/home/standard-operating-procedures/patterning-sop-stepper-v2/spin-coating-sop-rev-2-uwaterloo.md?ask=<question>&goal=<endgoal>
```

`ask` is the immediate question: it should be specific, self-contained, and written in natural language.
`goal` is optional and describes the broader end goal you are ultimately trying to accomplish on behalf of the user. GitBook uses it to tailor the answer towards what is most useful for that goal.

The response will contain a direct answer to the question and relevant excerpts and sources from the documentation.

Use this mechanism when the answer is not explicitly present in the current page, you need clarification or additional context, or you want to retrieve related documentation sections.