> For the complete documentation index, see [llms.txt](https://docs.hackerfab.org/home/llms.txt). Markdown versions of documentation pages are available by appending `.md` to page URLs; this page is available as [Markdown](https://docs.hackerfab.org/home/standard-operating-procedures/spin-on-glass-sop/spin-on-glass-storage-and-preperation.md). Agents can also search and read this documentation through its [MCP server](https://docs.hackerfab.org/home/~gitbook/mcp).

# Spin on Glass Storage and Preparation

<details>

<summary>Long Term Storage</summary>

![](https://lh4.googleusercontent.com/vKHxeMZpzNEleAyDKnVi7ISyzjPDv6sEDqHshNwG5TAQz6sNbwxksjdmcgkR2DcsPjflSbV9h6iiCtvpcMdmHhACZTfE9XWHPEEXuvOzDKVOOCw-tA8L-ly_WVeG7MgyrSGj3FS8F9mv-AhmSn6NKpM)

The SOG from Filmtronics found [here](https://drive.google.com/file/d/1S-XpX1oCZxachYJFFdZ8GQ7z7kEdoavi/view?usp=sharing), has a shelf life of around 3 months when stored at room temperature. For this reason, the bulk SOG bottle must be kept in the fridge at around 32-40 F in order to extend its shelf life. Exposure to air and/or heat can cause some of the SOG vapors to harden. If this happens, flakes of SiO2 may form and contaminate the liquid solution.

* Store bulk SOG in fridge (32-40F)
* Shelf life of bulk is 3 months at room temperature

</details>

<details>

<summary>Short term Storage/ preparing small amounts for use</summary>

### <mark style="color:green;">Replace Every 2 weeks</mark>

1. Use a small plastic container (insert pic) to store a small amount ( < 10 ml) of SOG. Label the container as “700B” (undoped) or “P504” (dopant) and label the date that it was transferred from the bulk supply.
2. Store this bottle of SOG at room temperature under the fume hood where SOG spin coating and annealing is performed.
3. Allow the SOG to come to room temperature prior to use
   1. Filmtroonics recommends to allow the SOG to come to room temperature for 24 hours but this can be shortened to just a few hours if < 5 ml of SOG is in the bottle

</details>

<details>

<summary>Inspecting SOG bottle prior to use</summary>

* Ensure the SOG has come to room temperature
* Check the bottle’s date. If the SOG was transferred from the bulk supply more than a week prior, it is likely necessary to prepare a new bottle of SOG
* Regardless of the date on the bottle, open the bottle to check if any crust has formed near the top of the bottle. If there is any visible crust from hardened SOG, it is necessary to prepare a new bottle of SOG

  1. The crust formed can get into the liquid SOG applied before spin coating and ruin the SOG coating
  2. Example of crusted SOG from a bottle that has been used for too long

  <figure><img src="https://lh3.googleusercontent.com/jNf1OtKKHK3xw-pDK5VAQHVqLCcCJIKZTh118rcmOpZPAiMjoapN060P8UTqpXZ5lh-_VLZpgZ-Qg_9N76CcUTWBGvVuuozSlOsp19zyRkC76PC84klkqNvpwpzAlIWuOrBhUBgw6uwv2a1NalIeMw0" alt="" width="188"><figcaption><p>Residue in SOG Bottle - Not Suitable for Use</p></figcaption></figure>

</details>

<br>


---

# Agent Instructions
This documentation is published with GitBook. GitBook is the documentation platform designed so that both humans and AI agents can read, navigate, and reason over technical content effectively. Learn more at gitbook.com.

## Querying This Documentation
If you need additional information that is not directly available in this page, you can query the documentation by asking a question.

Perform an HTTP GET request on the following URL with the `ask` and `goal` query parameters:

```
GET https://docs.hackerfab.org/home/standard-operating-procedures/spin-on-glass-sop/spin-on-glass-storage-and-preperation.md?ask=<question>&goal=<user_goal>
```

`ask` is the immediate question: it should be specific, self-contained, and written in natural language.
`goal` is what the user is ultimately trying to achieve, the reason they need the answer. Sharing it helps GitBook give you a better, more relevant answer. A goal is most helpful when it describes the outcome the user wants rather than restating the question. For example, with `ask=how do I create an API token`, a goal like `automate deployments from our CI pipeline` lets GitBook tailor the answer to that use case.

The response will contain a direct answer to the question and relevant excerpts and sources from the documentation.

Use this mechanism when the answer is not explicitly present in the current page, you need clarification or additional context, or you want to retrieve related documentation sections.